Table 3 Aggregate/binder ratio of mortars and sieve analysis results

From: Archaeometric characterization and restoration proposal for filling mortars of Oshki (Öşvank) church

Sample

Acid loss (%)

< 63 µm

63–125 µm

125–250 µm

250–500 µm

500–1000 µm

1000–2500 µm

2500–5000 µm

> 5000 µm

Loss

Remaining

H1

33.85

66.15

0.51

0.36

1.43

6.09

13.67

32.60

24.87

20.47

H2

29.61

70.39

0.39

0.39

1.47

5.33

10.40

28.77

15.99

37.26

H3

41.50

58.50

1.55

0.72

1.27

5.70

20.38

55.15

12.46

2.77

H4

37.67

62.33

1.23

0.51

1.46

5.66

20.15

53.40

15.76

1.83

H5

40.57

59.43

1.40

0.96

1.69

4.29

12.38

24.13

18.98

36.17

Average

36.64

63.36

1.02

0.59

1.46

5.41

15.40

38.81

17.61

19.70

  1. The values in the table indicate the proportions of aggregates passing the sieve